Crevice Corrosion in a Subsea System — Aspect Before Analysis

62 images
MMaterial
79 classified
PProduct
96 classified
Browse all Product →CCondition
84 classified
Browse all Condition →CmCapture method
52 classified
DfDetail focus
208 classified
Browse all Detail focus →Sharpest next filters
Browse by category (1)
Microstructure60
+52 more
and 12 more not shown here — refine in the Atlas
62 images

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Fractography by SEMDf - Fracture

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Brittle Fracture

ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Ductile Fracture

ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fractography by SEMDf - Corrosion

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
More from these cases

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Fractography by SEMDf - Brittle Cracks

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Fractography by SEMDf - Secondary Cracks

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Fractography by SEMDf - Fatigue Striation

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Intergranular Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Dimples

ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Dimples

ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Dimples

ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Cleavage Facets

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Cleavage Facets

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Fracture

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Dimples

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks
most recent

ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Aspect Before AnalysisDf - General View

ML00183 / Dec.2022
Ductile Behavior of an Aluminum Wheel
M - Aluminum Silicon MagnesiumP - CastingAp - AutomotiveCd - Ductile Behavior
Cm - Aspect Before AnalysisDf - General View

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Aspect Before AnalysisDf - General View

ML00181 / Apr.2022
Wear of a Carburized Hypoid Gear
M - Low Alloy for Thermochemical TreatmentP - Pinion-crown assemblyAp - ShipCd - Wear
Cm - Aspect Before AnalysisDf - General View

ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Aspect Before AnalysisDf - General View

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Field photoDf - General View

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - NItal Etched MacroDf - Seam

ML00176 / Nov.2021
Hydride Formation in a Titanium Blade
M - Unalloyed TitaniumP - BladeAp - Oil and GasCd - Hydride Formation
Cm - Aspect Before AnalysisDf - General View

ML00175 / Aug.2021
Localized External Wear of a Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Wear
Cm - Aspect Before AnalysisDf - General View

ML00174 / Jul.2021
Carburization of a 347 SS Welded Joint
M - Austenitic Stainless SteelP - Fabrication WeldAp - EnergyCd - Carburization
Cm - Field photoDf - General View

ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Microhardness identations