Rail
2 cases · 7 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00096 / Oct.2017
Carbon Steel Tee Rail
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Pearlite

ML00091 / Sep.2017
Flat Bottom Rail TR57
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Pearlite
More from these cases

ML00096 / Oct.2017
Carbon Steel Tee Rail
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Perlite

ML00096 / Oct.2017
Carbon Steel Tee Rail
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Transverse Section

ML00091 / Sep.2017
Flat Bottom Rail TR57
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Perlite

ML00091 / Sep.2017
Flat Bottom Rail TR57
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Transverse Section

ML00091 / Sep.2017
Flat Bottom Rail TR57
M - High Strength Low AlloyP - RailAp - TransportationCd - Typical manufacturing
Cm - Transverse Section AspectDf - General View