Crevice Corrosion in a Subsea System — Aspect Before Analysis

27 images
MMaterial
79 classified
Browse all Material →PProduct
96 classified
Browse all Product →CCondition
84 classified
Browse all Condition →CmCapture method
52 classified
DfDetail focus
208 classified
Browse all Detail focus →Sharpest next filters
Browse by category (1)
Standard69
+61 more
and 21 more not shown here — refine in the Atlas
27 images

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00161 / Mar.2020
Brittle Fracture of a High Strength Socket
M - Medium Carbon Tool SteelP - ToolAp - Oil and GasCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Brittle Fracture

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture

ML00127 / May.2018
Hydrogen Cracks of Cadmium Plated Studs
M - Low Alloy Medium Carbon QTP - Allen StudAp - Oil and GasCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Fracture

ML00126 / Mar.2018
Hydrogen Fracture of Subsea Allen Bolts
M - Low Alloy Medium Carbon QTP - Coated ProductAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Fracture
More from these cases

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00161 / Mar.2020
Brittle Fracture of a High Strength Socket
M - Medium Carbon Tool SteelP - ToolAp - Oil and GasCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Intergranular Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Dimples

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks

ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - General View

ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture

ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture

ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Ductile Fracture

ML00127 / May.2018
Hydrogen Cracks of Cadmium Plated Studs
M - Low Alloy Medium Carbon QTP - Allen StudAp - Oil and GasCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking

ML00126 / Mar.2018
Hydrogen Fracture of Subsea Allen Bolts
M - Low Alloy Medium Carbon QTP - Coated ProductAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Ductile Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Intergranular Cracking
most recent

ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Aspect Before AnalysisDf - General View

ML00183 / Dec.2022
Ductile Behavior of an Aluminum Wheel
M - Aluminum Silicon MagnesiumP - CastingAp - AutomotiveCd - Ductile Behavior
Cm - Aspect Before AnalysisDf - General View

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Aspect Before AnalysisDf - General View

ML00181 / Apr.2022
Wear of a Carburized Hypoid Gear
M - Low Alloy for Thermochemical TreatmentP - Pinion-crown assemblyAp - ShipCd - Wear
Cm - Aspect Before AnalysisDf - General View

ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Aspect Before AnalysisDf - General View

ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Field photoDf - General View

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - NItal Etched MacroDf - Seam

ML00176 / Nov.2021
Hydride Formation in a Titanium Blade
M - Unalloyed TitaniumP - BladeAp - Oil and GasCd - Hydride Formation
Cm - Aspect Before AnalysisDf - General View

ML00175 / Aug.2021
Localized External Wear of a Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Wear
Cm - Aspect Before AnalysisDf - General View

ML00174 / Jul.2021
Carburization of a 347 SS Welded Joint
M - Austenitic Stainless SteelP - Fabrication WeldAp - EnergyCd - Carburization
Cm - Field photoDf - General View

ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Microhardness identations