Crevice Corrosion in a Subsea System — Aspect Before Analysis

39 images

M

Material

79 classified

Browse all Material →
P

Product

96 classified

Browse all Product →
Ap

Application

37 classified

Browse all Application →
C

Condition

84 classified

Browse all Condition →
Cm

Capture method

52 classified

Browse all Capture method →
Df

Detail focus

208 classified

Browse all Detail focus →

Sharpest next filters

Browse by category (1)
39 images
Aspect of the internal side of the drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained uncleaned for a period a little longer than 1 month.
775
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Internal Surface
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the localized corroded regions in form of pits.
1228
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
163
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - General View
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
125
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Localized Corrosion
Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Transverse Section

+13 more from this case →

ML00121 — Pitting Corrosion in a Subsea SystemM - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Aspect of the Nitronic 60 cylinder, OD 36.4mm, presenting pits at the external surface.
219
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - External Surface
Nitronic 60 cylinder. Detailed aspect of the pitting in a low magnification microscope.
197
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface AspectDf - Pitting
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, and evidences of the manufacturing process by hot forming.
179
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, with some aligned non metallic inclusions.
157
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrographic detail of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, typical of a solution annealed condition.
136
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite

+14 more from this case →

most recent

The location of the threaded fitting started leaking after less than five years in service. 
Although the corrosion rate was not high, the localized material loss in the threaded surface of the carbon steel flange allowed the connection leakage.
770
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Aspect Before AnalysisDf - General View
Front wheel 17 x 7J of a passenger vehicle (identified as WHEEL 1) that broke during a car accident on a road.
1645
ML00183 / Dec.2022
Ductile Behavior of an Aluminum Wheel
M - Aluminum Silicon MagnesiumP - CastingAp - AutomotiveCd - Ductile Behavior
Cm - Aspect Before AnalysisDf - General View
Tool fixture 5" long, nominal diameter 2", presenting a recess 1/2" deep from two sides.  The rupture occurred about 2" from the end of the rod.   Scale in milimeters.
523
ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Aspect Before AnalysisDf - General View
Pinion of hypoid gearbox, assembled in a 1560-mm long shaft that operated during more than 60,000 hours, and removed from service due to unacceptable wear damage.
1028
ML00181 / Apr.2022
Wear of a Carburized Hypoid Gear
M - Low Alloy for Thermochemical TreatmentP - Pinion-crown assemblyAp - ShipCd - Wear
Cm - Aspect Before AnalysisDf - General View
Aspect of the 3 1/2" diameter tube after the water leakage in high temperature.
963
ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Aspect Before AnalysisDf - General View
2" drain line from the main 10" line. The leakage occurred at the margin of the weld, a short time after the introduction of the reinforced ribs to reduce vibration.
642
ML00179 / Feb.2022
Hydrides in Titanium Weld
M - Unalloyed TitaniumP - In Field WeldAp - Chemical IndustryCd - Hydride Formation
Cm - Field photoDf - General View
The drilling connector, 21" diameter, presented a crack at the margin of the weld in the forging side (left side of the weld in the figure).
748
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View
Macrography of the longitudinally seam weld of the 24" diameter tube, showing that it was welded from both sides and there is a segregation line in the center of the tube thickness.
737
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - NItal Etched MacroDf - Seam
The titanium rotor blade of a flowmeter broke after two years in service in an acid environment, containing H2S.
340
ML00176 / Nov.2021
Hydride Formation in a Titanium Blade
M - Unalloyed TitaniumP - BladeAp - Oil and GasCd - Hydride Formation
Cm - Aspect Before AnalysisDf - General View
Aspect of the wire rope, 1 1/2" diameter, presenting regions of flattened  areas at the surface of the outer wires. It is a 6 x 19 Seale construction, right regular lay.
553
ML00175 / Aug.2021
Localized External Wear of a Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Wear
Cm - Aspect Before AnalysisDf - General View
The carcass was manufactured using niobium stabilized plates, grade AISI 347, with circumferential welds, where the through wall cracks were detected.
303
ML00174 / Jul.2021
Carburization of a 347 SS Welded Joint
M - Austenitic Stainless SteelP - Fabrication WeldAp - EnergyCd - Carburization
Cm - Field photoDf - General View
Aged microstructure of the HP stainless steel, modified with 1%Nb, cast fitting, tubular, operating for 6 years in a furnace which design temperature is 1100°C.  The material presented a network of primary carbides, white and grey, and an austenitic matrix with coalescing secondary precipitation. Some voids. The Vickers identation indicates a hardness value about 260HV 100g in the aged austenitic matrix.
493
ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Microhardness identations
TECMETAL