High Mn Austenitic Steel

1 case · 19 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the internal side of the drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained uncleaned for a period a little longer than 1 month.
775
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Internal Surface

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
163
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - General View
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
125
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Localized Corrosion
Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Transverse Section

+13 more from this case →