Ferrous Alloys
9 cases · 138 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Ferrous Alloys — sub-branches

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Longitudinal Section

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - NItal Etched MacroDf - Fracture

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Aspect Before AnalysisDf - Fracture

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Aspect by NDTDf - Cracks

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Aspect by NDTDf - Cracking

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - NItal Etched MacroDf - Cracking
More from these cases

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - External Surface

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect by NDTDf - Cracking

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Identification drawingDf - Longitudinal Section

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Identification drawingDf - Fracture

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Identification drawingDf - Welded Joint

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Identification drawingDf - Fracture

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Identification drawingDf - Welded Joint

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Surface AspectDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Ferrite and Bainite

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Bainite

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Aspect Before AnalysisDf - Welded Joint

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Aspect Before AnalysisDf - Fracture

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Aspect by NDTDf - Cracking

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital etched, OMDf - Intergranular Cracking

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital etched, OMDf - Intergranular Cracking

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks