Damage

3 cases · 22 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
125
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Localized Corrosion
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the localized corroded regions in form of pits.
1228
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Transverse section of the 2" diameter pipe at the pitting location.  The pipe was leaking.
1323
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Transverse Section AspectDf - Pitting

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion

+1 more from this case →

ML00121 — Pitting Corrosion in a Subsea SystemM - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Nitronic 60 cylinder. Detailed aspect of the pitting in a low magnification microscope.
197
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface AspectDf - Pitting
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the structure revealed by dissolution of the material (inside the pits) evidencing the strain hardened layer that is presented at the cylinder surface due to the manufacturing process.
106
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Nitronic 60 cylinder. Scanning electron microscopy image detail of a corroded region inside a pitting showing the etched structure (strain hardened austenitic structure).
103
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
17-4 PH rod. Detailed aspect of the pitting in a low magnification microscope.
115
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface AspectDf - Pitting

+3 more from this case →

ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
The external surface of the 2" diameter pipe is rusted and the leakage is associated to “holes” that appear very small at the surface but that open a large hole in the middle of the thickness.
507
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting
Micrography of a transverse section of the pipe, presenting the pitting corrosion. As polished.
310
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OMDf - Pitting