Back to Austenitic Stainless Steel
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.

Associated Images
Transverse section of the 2" diameter pipe at the pitting location.  The pipe was leaking.
1323
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Transverse Section AspectDf - Pitting
The external surface of the 2" diameter pipe is rusted and the leakage is associated to “holes” that appear very small at the surface but that open a large hole in the middle of the thickness.
507
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting
Micrography of a transverse section of the pipe, presenting the pitting corrosion. As polished.
310
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OMDf - Pitting
Austenitic structure at the transverse section of the pipe, free from carbides.
277
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Austenitic structure, free from carbides, exactly in the region of the pitting, indicating that the corrosion is not associated to the material microstructure.
261
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite