Back to Austenitic / Martensitic
ML00121 - Feb.2018

Pitting Corrosion in a Subsea System

Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region in a pit, at the external surface of the cylinder.  The corrosion (dissolution) revealed the strain hardened layer at the surface.

Associated Images
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the localized corroded regions in form of pits.
1228
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Aspect of the Nitronic 60 cylinder, OD 36.4mm, presenting pits at the external surface.
219
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - External Surface
Nitronic 60 cylinder. Detailed aspect of the pitting in a low magnification microscope.
197
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface AspectDf - Pitting
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, and evidences of the manufacturing process by hot forming.
179
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, with some aligned non metallic inclusions.
157
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrographic detail of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, typical of a solution annealed condition.
136
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrography of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a shadow close to the external surface that is associated to a small layer of strain hardened structure (deformation twins).
133
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened
Nitronic 60 cylinder. Micrography of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a 0.15mm layer of strain hardened structure (deformation twins).
120
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened
Nitronic 60 cylinder. Micrographic detail of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a layer of strain hardened structure (deformation twins).
113
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the structure revealed by dissolution of the material (inside the pits) evidencing the strain hardened layer that is presented at the cylinder surface due to the manufacturing process.
106
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Nitronic 60 cylinder. Scanning electron microscopy image detail of a corroded region inside a pitting showing the etched structure (strain hardened austenitic structure).
103
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Aspect of the 17-4 PH rod, OD 10.6 mm, presenting deep pits at the external surface.
125
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - External Surface
17-4 PH rod. Detailed aspect of the pitting in a low magnification microscope.
115
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface AspectDf - Pitting
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Kalling Etched MacroDf - Pitting
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Kalling Etched Micrography by OMDf - Martensite
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Kalling Etched Micrography by OMDf - Martensite
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Kalling Etched Micrography by OMDf - Martensite
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Kalling Etched Micrography by OMDf - Pitting
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting