Back to Low Alloy Medium Carbon QT
Micrographic detail of the fatigue cracking, straight and without microstructural influence.

Associated Images
General view of the cylindrical valve body, 6 5/8" nominal diameter, showing a transverse straight crack at the external surface.
406
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - General View
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - Longitudinal Section
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect by NDTDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect by NDTDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Longitudinal Section AspectDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Longitudinal Section AspectDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack