Back to Low Alloy Medium Carbon QT
Micrography in low magnification, as polished, of the crack in the valve thickness,  showing the straight aspect of the fatigue propagation.

Associated Images
General view of the cylindrical valve body, 6 5/8" nominal diameter, showing a transverse straight crack at the external surface.
406
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - General View
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect Before AnalysisDf - Longitudinal Section
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect by NDTDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Aspect by NDTDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Longitudinal Section AspectDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Repair
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - NItal Etched MacroDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Nital Etched Micrography by OMDf - Fatigue Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - Longitudinal Section AspectDf - Crack
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Hot cracking
ML00162 / Apr.2020
Valve Body Crack Growth from Weld Defects
M - Low Alloy Medium Carbon QTP - Valve BodyAp - O&G Well DrillingCd - Fatigue Induced by a Defect
Cm - As polished micrographyDf - Fatigue Crack