Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrography of the plate in a longitudinal section, presenting a typical ferritic pearlitic structure, banded.  The plate is 22 mm thick.
182
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Strain hardened pearlite
ML00110 / Jan.2018
Non Conformance in Spray and Fuse Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Heat Treatment Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrographic detail of a transverse section of the tubing, in the center of the thickness. Ferritic-pearlitic structure. Pearlite colonies in bands.
401
ML00116 / Jan.2018
CMn Steel Structural Tubing 6 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrographic detail of a transverse section of the 5 mm thick tubing, in the center of the thickness. Ferritic-pearlitic structure, with the pearlite presenting a coalesced aspect.  The tubing was in service at ambient temperature, painted, and the coalesced aspect was generated before service, perhaps during the tubing manufacturing.
393
ML00115 / Jan.2018
CMn Steel Structural Tubing 5 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrographic detail of a transverse section of the tubing, in the center of the thickness.  
Ferritic-pearlitic structure. 
Pearlite colonies in bands.
346
ML00114 / Jan.2018
CMn Steel Structural Tubing 8 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrographic detail of a longitudinal section of a 4 mm diameter wire, presenting an aligned and highly strained pearlitic structure. Base metal.
386
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Strain hardened pearlite
Micrography of a transverse section of the pipe, external diameter 33.4 mm schedule XXS, in the center of the 9.1 mm thickness.  The structure is predominantly ferritic.  Small amount of pearlite.
556
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic

More from these cases

ML00119 — Thermal Fatigue of a Marine BoilerM - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Micrography of the plate in a longitudinal section, presenting a typical ferritic pearlitic structure, banded.
165
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrographic detail of the ferritic pearlitic structure of the plate in the longitudinal section.
147
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrography of the weld metal in the center os the weld. Columnar grains (of the previous austenite) with primary ferrite in the grain boundaries and acicular ferrite intragranular.
125
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Ferritic Weld Metal
Micrographic detail of the weld metal in the center os the weld. Columnar grains (of the previous austenite) with primary ferrite in the grain boundaries; and details of the ferrite with aligned second phases and acicular ferrite, intragranular.
112
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Ferritic Weld Metal
Micrography of the tube HAZ in a region of (austenitic) grain coarse, presenting a bainitic structure.
105
ML00119 / Feb.2018
Thermal Fatigue of a Marine Boiler
M - Low Carbon SteelP - Fabrication WeldAp - ShipCd - Thermal Fatigue
Cm - Nital Etched Micrography by OMDf - Bainitic HAZ

+6 more from this case →

ML00117 — High Carbon Steel Wire RopeM - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - No Coating Layer
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Strain hardened pearlite
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - No Coating Layer
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Strain hardened pearlite
ML00117 / Jan.2018
High Carbon Steel Wire Rope
M - High Carbon SteelP - Wire RopeAp - Oil and GasCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - No Coating Layer
ML00110 — Non Conformance in Spray and Fuse PinM - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Heat Treatment Defect
ML00110 / Jan.2018
Non Conformance in Spray and Fuse Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Heat Treatment Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00110 / Jan.2018
Non Conformance in Spray and Fuse Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Heat Treatment Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00116 — CMn Steel Structural Tubing 6 mm thickM - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
ML00116 / Jan.2018
CMn Steel Structural Tubing 6 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00115 — CMn Steel Structural Tubing 5 mm thickM - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
ML00115 / Jan.2018
CMn Steel Structural Tubing 5 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00114 — CMn Steel Structural Tubing 8 mm thickM - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
ML00114 / Jan.2018
CMn Steel Structural Tubing 8 mm thick
M - CMn SteelP - Seamless Round ShapeAp - StructureCd - Removed From Service
Cm - Nital Etched Micrography by OMDf - Banded Structure
ML00113 — Autogenous Weld of a Carbon Steel WireM - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Martensite
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Martensite
ML00112 — 1" XXS Pipe Not Qualified For Low TempM - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic