Fabrication Defect
10 cases · 36 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Fabrication Defect — sub-branches

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Granular structure

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Banded Structure

ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - NaOH Electrolytic Etched MicroDf - Ferrite and Austenite

ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic

ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00099 / Jan.2018
Forging Defect in a Cadmium Plated Nut
M - Medium Carbon SteelP - NutAp - PipingCd - Fabrication Defect
Cm - Nital Etched Micrography by OMDf - Martensite

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Martensite
More from these cases

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Martensite

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Grain refined structure

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainitic HAZ

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Bainite

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainitic HAZ

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainite

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Banded Structure

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Banded Structure

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Martensite

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Banded Structure

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Banded Structure

ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - NaOH Electrolytic Etched MicroDf - Ferrite and Austenite

ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic

ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic

ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00099 / Jan.2018
Forging Defect in a Cadmium Plated Nut
M - Medium Carbon SteelP - NutAp - PipingCd - Fabrication Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line