Scanning Electron Microscope

4 cases · 16 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the localized corroded regions in form of pits.
1228
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Tempered martensitic microstructure of the knife observed in a transverse section micrography.  There are also secondary carbides (white globules) that increase the material wear resistance.
254
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Kalling Etched Micrography by SEMDf - Martensite
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00121 — Pitting Corrosion in a Subsea SystemM - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Nitronic 60 cylinder. Scanning electron microscopy image of a corroded region at the external surface of the cylinder, that is austenitic.  The image shows the structure revealed by dissolution of the material (inside the pits) evidencing the strain hardened layer that is presented at the cylinder surface due to the manufacturing process.
106
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
Nitronic 60 cylinder. Scanning electron microscopy image detail of a corroded region inside a pitting showing the etched structure (strain hardened austenitic structure).
103
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting
ML00054 — Cutlery CorrosionM - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Detail of the tempered martensitic microstructure with secondary carbides of the knife, observed in a transverse section micrography.
206
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Kalling Etched Micrography by SEMDf - Martensite
Aspect of the rusted surface after cleaning, showing adhered products at the surface, in regions where the passive layer was destroyed and pitting corrosion occurred.
184
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Detail of the rusted surface. EDS analysis inside the pitting shows a high Cl peak (the bright aspect inside the pitting), indicating that the salt over the surface was responsible for destroying the passive layer and the localized corrosion occurred.
172
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Micrographic aspect of the pitting corrosion at the knife surface.  It is possible to see the typical pitting aspect of a localized corrosion that appears as a small dot at the surface but it is a big crater under the surface.
185
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Micrography by SEMDf - Pitting
Detail of the micrographic aspect of the pitting corrosion at the knife surface.
168
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Micrography by SEMDf - Pitting
ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting