Back to Martensitic Stainless Steel
Micrographic detail of the defect (void in the right side of the figure), as polished.  In the left side it is the surface of the water blade and there are some non metalic inclusions in this region.

Associated Images
Casting defect identified in the micrographic section, as polished, of the sample removed from the blade. The total lenght of the defect detected by magnetic particle during inspection is 10 mm.
1041
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Micrography by SEMDf - Void
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Aspect Before AnalysisDf - Crack
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched MacroDf - Crack
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Micrography by OMDf - Void
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Micrography by OMDf - Non Metallic Inclusions
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched Micrography by OMDf - Delta Ferrite Islands
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched Micrography by OMDf - Coarse Structure
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched Micrography by OMDf - Delta Ferrite Islands
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched Micrography by OMDf - Void
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Micrography by SEMDf - Void
ML00017 / Apr.2017
Casting Defect in CA6NM
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Casting Defect
Cm - Kalling Etched Micrography by OMDf - Non Metallic Inclusions