Crevice Corrosion in a Subsea System — Aspect Before Analysis

Fractured position of the casting cylinder of 10.5 mm thickness (minimum measured thickness) showing a brittle behavior (lack of plastic deformation), typical of overloading a material with 1% ductility (measured in the tensile test). This is the view of the internal surface of the cylinder, presenting regions of localized thinning in this surface that was in contact with (treated) cooling water.  The external side of the cylinder was painted.
918
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fracture Surface AspectDf - General View
The camshaft broke in a brittle way in a region where the shaft changed the geometry, close to a chilled lobe.
550
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - Aspect Before AnalysisDf - Fracture
Grey cast iron microstructe. Perlitic matrix and graphite flakes.
508
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Pearlite Matrix

More from these cases

ML00141 — Brittle Fracture of a Corroded Gray Cast IronM - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Fracture aspect of the casting cylinder at the 10.5 mm thickness, showing a brittle behavior (lack of plastic deformation). The internal side of the cylinder is to the top of the figure, and the painted surface is to the bottom of the figure.
129
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fracture Surface AspectDf - Brittle Fracture
Detailed aspect of the cylinder fracture, the internal surface to the top of the figure and the painted external surface to the bottom of the figure.
103
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fracture Surface AspectDf - Brittle Fracture
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - NItal Etched MacroDf - Brittle Fracture
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - As polished micrographyDf - Close to the Internal Surface
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - As polished micrographyDf - In the Center of the Thickness

+30 more from this case →

ML00060 — Brittle Fracture of a Chilled Cast Iron CamshaftM - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - NItal Etched MacroDf - Longitudinal Section
Close to the camshaft lobe surface, the chilled casting presents a white cast iron structure. Primary carbides and ledeburite with a hardness level about 50 HRc.
102
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Close to the External Surface
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Close to the External Surface
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - In the Center of the Thickness
ML00060 / Apr.2017
Brittle Fracture of a Chilled Cast Iron Camshaft
M - Chilled Cast IronP - ShaftAp - AutomotiveCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - In the Center of the Thickness

+5 more from this case →

ML00032 — Cast Iron Case of Drilling EquipmentM - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Low magnification micrography presenting the grapjite morphology.
138
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Micrography by OMDf - Graphite Type A (ASTM A247)
Grey cast iron structure.  As polished.
110
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Micrography by OMDf - Graphite in Flakes
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Micrography by OMDf - Graphite in Flakes
Grey cast iron with graphite in flakes and perlitic matrix.
110
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Perlite Matrix
ML00032 / Jan.2017
Cast Iron Case of Drilling Equipment
M - Gray Cast ironP - CastAp - O&G Well DrillingCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Graphite Type A (ASTM A247)