Atlas

9 cases · 63 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Longitudinal Section
Micrography of the tranverse section of the tube, in the center of the thickness.  There are small grains and large grains, characterizing a dual grain size.  The large grains size is about 100 microns, more than 10 times larger than the average size of the smaller grains size.
101
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - FeCl3+HCl+H2O Etched MicroDf - Dual grain sizes
Optical micrography of a longitudinal section of the fractured bolt, at the thread.  The material is austenitic, free from carbides, and the threads were almost removed by the stress corrosion cracks.
756
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks
Micrography of the plate material presenting a granular austenitic structure, free from precipitation.
122
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Eletrolytically Etched Micrography by OMDf - Austenite
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Typical branched stress corrosion cracks in a low carbon steel, ferritic-pertlitic structure. The cracks are filled with corrosion products.
771
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
A small sample was removed from the steam drum and the micrography shows that the cracks are intergranular (previous austenite) and located in the weld metal.
285
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Localized Corrosion

More from these cases

ML00168 — SCC of Austenitic SS Flange Stub EndM - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - As polished micrographyDf - Close to the External Surface
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - As polished micrographyDf - Multiple cracks
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Close to the External Surface

+4 more from this case →

ML00165 — SCC of Aluminum Bronze Heating CoilM - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - FeCl3+HCl+H2O Etched MicroDf - Alpha
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - As polished micrographyDf - Cracking
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - As polished micrographyDf - Intergranular Corrosion
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - As polished micrographyDf - Through Wall Cracking
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - FeCl3+HCl+H2O Etched MicroDf - External Surface

+4 more from this case →

ML00157 — Bolts Under Chloride SCC ConditionsM - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Low magnification micrography, by optical microscope, of the longitudinal section of a damaged bolt, in the center of the thickness. The microstructure is austenitic, free from carbides.
100
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Strain Hardened
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Strain Hardened
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks

+2 more from this case →

ML00051 — Chloride SCC of 316 Heat Exchanger PlateM - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Micrographic detail of the austenitic microstructure of the heat exchanger plate, free from carbides that suggest the adoption of a material in a solution annealed condition, although the high hardness level indicates cold working.
109
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Eletrolytically Etched Micrography by OMDf - Austenite
Micrography presenting the transgranular morphology of the stress corrosion cracks of the austenitic plate.  EDS analysis at the plate surface indicated high Cl peaks.
111
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Eletrolytically Etched Micrography by OMDf - Corrosion Cracking
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Corrosion Cracking
ML00019 — Transgranular SCC in Boiler Steam DrumM - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
Micrographic detail of the transgranular stress corrosion cracking.
157
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
ML00018 — SCC in Boiler Steam DrumM - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Ferritic perlitic structure of the shell plate.
207
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrography of the crack at the internal surface of the steam drum.  The shell plate presents a ferritic perlitic structure.
162
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
Micrography of a crack, in a sample as polished, presenting the opened crack.
144
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Micrography by OMDf - Branched Cracks
Stress corrosion cracks propagating in the ferritic-perlitic structure.
120
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
Micrography of a crack, as polished, presenting the cracks filled with corrosion products.
100
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Micrography by OMDf - Branched Cracks

+2 more from this case →

ML00020 — Intergranular SCC in Boiler Steam Drum RepairM - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
The micrography of the small sample removed from the steam drum shows that the cracks are intergranular (previous austenite) and located in the weld metal.
274
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Secondary cracks in the weld metal showing an intergranular morphology. Stress Corrosion Cracking.
249
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the secondary cracks in the weld metal with intergranular morphology. Stress Corrosion Cracking.
251
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the intergranular stress corrosion cracking of the drum shell weld repair.
217
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
ML00016 — SCC in Free Cutting 303SSM - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Non Metallic Inclusions
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Localized Corrosion
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Branched Cracks