A

3 cases · 19 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

A — sub-branches

Micrography of a transverse section of the pipe, external diameter 33.4 mm schedule XXS, in the center of the 9.1 mm thickness.  The structure is predominantly ferritic.  Small amount of pearlite.
556
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic
Micrography of a transverse section of the pipe, external diameter 26.7 mm, in the center of the 7.85mm thickness.  Refined structure but not uniform.  Ferrite and pearlite.
512
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Micrography of a transverse section of the pipe, presenting the pitting corrosion. As polished.
310
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OMDf - Pitting

More from these cases

ML00112 — 1" XXS Pipe Not Qualified For Low TempM - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the External Surface
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the External Surface
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Predominantly Ferritic
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the Internal Surface
ML00112 / Dec.2017
1" XXS Pipe Not Qualified For Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the Internal Surface

+2 more from this case →

ML00111 — 3/4" XXS Pipe Not Qualified for Low TempM - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the Internal Surface
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the Internal Surface
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the External Surface
ML00111 / Dec.2017
3/4" XXS Pipe Not Qualified for Low Temp
M - Low Carbon SteelP - Seamless PipeAp - RefineryCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Close to the External Surface

+2 more from this case →

ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Austenitic structure at the transverse section of the pipe, free from carbides.
277
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Austenitic structure, free from carbides, exactly in the region of the pitting, indicating that the corrosion is not associated to the material microstructure.
261
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite