312

2 cases · 17 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

312 — sub-branches

The scanning electron microscopy image of the internal surface of the tube in position 2 shows a localized  corrosion region with intergranular morphology, as well a crack from the corroded region.
1237
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Surface Aspect by SEMDf - Intergranular Corrosion
Transverse section of the 2" diameter pipe at the pitting location.  The pipe was leaking.
1323
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Transverse Section AspectDf - Pitting

More from these cases

ML00086 — Intergranular Corrosion of Sensitized 304SSM - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in the colder part of the equipment, position 1.  The material presented carbide precipitation at grain boundaries (not yet fully surrounding the grains) and at this point the tube presented no internal corrosion.
338
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in position 2, where the temperature was higher and the carbide precipitation increased during service.
272
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intergranular Precipitation
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in position 3, where intergranular and transgranular carbide precipitation occurred during service.
234
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intragranular Secondary Precipitation
The low magnification image of the internal surface of the tube, in position 2, shows several points of localized corrosion, with intergranular morphology.
193
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Surface Aspect by SEMDf - Intergranular Corrosion
Micrography of a longitudinal section of the tube in position 2, presenting thinning by intergranular corrosion at the internal surface.
193
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intergranular Corrosion

+3 more from this case →

ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
The external surface of the 2" diameter pipe is rusted and the leakage is associated to “holes” that appear very small at the surface but that open a large hole in the middle of the thickness.
507
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting
Micrography of a transverse section of the pipe, presenting the pitting corrosion. As polished.
310
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OMDf - Pitting

+2 more from this case →