Ferritic pearlitic

1 case · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrography of a longitudinal section of the shell plate base metal, presenting a typical ferritic-perlitic microstructure.
149
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

More from these cases

ML00008 — Cold Cracks in CMn Steel Pressure VesselM - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Higher magnification of the ferritic-perlitic microstructure of the shell plate in the longitudinal section.
129
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ.
123
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. The cracks are mainly located at the fusion line.
118
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. Several internal cracks at the fusion line.
101
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

+1 more from this case →