Martensitic Stainless Steel

2 cases · 18 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

The as polished micrographic aspect of the corroded surface shows pitting and several microcracks, probably associated to the biological attack and material embrittlement.  Replication technique.
924
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - As polishedDf - Microcracks
13Cr SS longitudinal section micrography, at the collapsed region, showing a ferritic matrix structure (overtempered) with the previous austenite grain boundaries decorated by phases (carbides and probably martensite islands), indicating that the material was exposed to a high tempering temperature that created a partial austenitizing condition. It explains the material low toughness and lower strenght (than required).
436
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section

More from these cases

ML00092 — MIC of a Valve BodyM - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - Corrosion
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - Internal Surface
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - Localized Corrosion
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - Surface AspectDf - Localized Corrosion
ML00092 / Sep.2017
MIC of a Valve Body
M - Martensitic Stainless SteelP - Valve BodyAp - Oil and GasCd - Brittle Behavior
Cm - Kalling etched, OMDf - Martensite

+3 more from this case →

ML00039 — Collapse in Tubular 13CrM - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Prior Austenite Boundaries Decorated
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Transverse Section
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Transverse Section
ML00039 / Apr.2017
Collapse in Tubular 13Cr
M - Martensitic Stainless SteelP - Seamless PipeAp - Oil and GasCd - Heat Treatment Defect
Cm - Kalling Etched Micrography by OMDf - Overtempered Structure

+3 more from this case →