Longitudinal Section
3 cases · 6 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00106 / Dec.2017
Inconel 718 Submarine Bolt
M - NiCrFe AlloyP - BoltAp - SubseaCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section

ML00105 / Jun.2018
Inconel 718 Bolt of Special Head
M - NiCrFe AlloyP - FastenerAp - SubseaCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section

ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
More from these cases

ML00106 / Dec.2017
Inconel 718 Submarine Bolt
M - NiCrFe AlloyP - BoltAp - SubseaCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section

ML00105 / Jun.2018
Inconel 718 Bolt of Special Head
M - NiCrFe AlloyP - FastenerAp - SubseaCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section

ML00105 / Jun.2018
Inconel 718 Bolt of Special Head
M - NiCrFe AlloyP - FastenerAp - SubseaCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section