Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrography of a longitudinal section, in the center, of the broken 5/8" bolt, presenting an aged martensitic structure. There are vertical "lines" that correspond to segregation bands due to the forming direction.  These bands are evident only using low magnification microscopy.
168
ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Longitudinal Section
The fracture of the bolt occurred associated to the bottom of the thread. Compare this photo with the previous one to understand where the fracture started.
115
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Nital Etched Micrography by OMDf - Longitudinal Section
ML00093 / Sep.2017
MIC of a Drilling Tool
M - Low Alloy Medium Carbon QTP - Heat Treated PartAp - O&G Well DrillingCd - Brittle Behavior
Cm - Nital Etched Micrography by OMDf - Longitudinal Section

More from these cases

ML00139 — Hydrogen Fracture of a 17-4 PH Allen BoltM - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - As polished micrographyDf - Longitudinal Section
ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Longitudinal Section