Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Fusion Line
ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Fusion Line
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Fusion Line

More from these cases

ML00173 — Welding Cracks in an Aged HP Cast FittingM - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Fusion Line
Same region as the previous figure, showing the structure of the base metal and weld metal, at the cracked area.  In the base metal, the cracks are associated to the primary carbides network and in the weld metal it is associated to the solidification columnar grains.
110
ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Fusion Line
ML00052 — Cold Cracks in API 5CT L80 Tube Welded to a Structural PartM - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Fusion Line
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Fusion Line
ML00026 — Autogenous Seam Welded Tube in Ferritic SSM - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Fusion Line