Damage

8 cases · 28 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Intergranular Cracking
Micrography of the weld metal presenting a martensitic island with microcracks, due to a localized increase in the manganese and silicon content, probably because an active flux was adopted in a condition where a high cleanning action was not required. A high flux-to-wire ratio (>1) could also be an issue.
794
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Hard Spots
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ.
123
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Micro by OM, picric acid+FeCl3+H2O etchDf - Segregated Regions

More from these cases

ML00072 — Liquation Cracks in a High Strength JointM - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00071 — Reheating Cracking of a CrMo Vessel WeldM - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00067 — Cold Cracks in C-Mn SAW Weld MetalM - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00069 — Liquation Cracks in SAW of Low Carbon SteelM - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Intergranular Cracking
Micrography of the fractured region, from the weld metal side, showing that the intergranular cracking occurred at the coarse grain heat affected zone. The structure is bainitic and there are segregated regions in the previous austenite grain boundaries.
127
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Intergranular Cracking
ML00010 — Cold Cracks in a Gouged Weld MetalM - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Hard Spots
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Hard Spots
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Hard Spots
ML00008 — Cold Cracks in CMn Steel Pressure VesselM - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. The cracks are mainly located at the fusion line.
118
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. Several internal cracks at the fusion line.
101
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell using an unsuitable welding procedure, with a low preheating and no PWHT. Cracks propagated in the weld metal.
100
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00013 — Welding Cracks in Mooring ChainM - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Segregated Regions