Welding Defect

3 cases · 53 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

The drilling connector, 21" diameter, presented a crack at the margin of the weld in the forging side (left side of the weld in the figure).
745
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View
The macrography of a longitudinal section of the pipe and connector, at the welded joint, shows that the welding was conducted from both side of the groove, starting from the ID and finishing from the OD, ID later machined flush. The cracking was detected by ultrasonic test and the macro shows that it is at the fusion line, growthing into the weld metal. See the schematic drawing in the next figure
535
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Longitudinal Section
The repair weld presented several cracks in the weld metal, transverse to the weld, detected during inspection using magnetic particle test.  The cracks were mainly located in regions of the structure where the repair was conducted by welding in the vertical position using 1/8" stick electrode.
710
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Aspect by NDTDf - Cracking

More from these cases

ML00178 — Cold cracks in Cr-Mo Welded ForgingM - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Circumferential weld aspect. Two passes in the cap. This forging to pipe welded joint, 22 mm thick, was welded by an automatic process in a narrow gap.  The pipe is to the top of the image and the forging is to the bottom of the image.
165
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - External Surface
The dye check image shows the detected crack, 50 mm long, at the margin of the weld in the forging side.
137
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect by NDTDf - Cracking
Macrography of the welded joint between the forging and the pipe, showing it was welded in a narrow gap, indicating by the arrow the location of the crack at the margin of the weld, in the forging side.
129
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint
Quenched and tempered structure of the F22 steel forging, presenting about 230HV10 average hardness.
133
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal
Tempered martensitic structure for the F22 forging base metal.
129
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite

+14 more from this case →

ML00072 — Liquation Cracks in a High Strength JointM - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Schematic drawing presenting the longitudinal section of the pipe and connector at the welded joint
105
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Identification drawingDf - Longitudinal Section
Hot cracking at the fusion line of the connector side, in a welded joint between a forging and a pipe, in a macrographic sample.  The region of the heat affected zone of the connector presents a dendritic aspect suggesting that the forging reduction rate of the connector was not too high and did not broke the cast structure.
110
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - NItal Etched MacroDf - Welded Joint
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Aspect Before AnalysisDf - General View
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

+11 more from this case →

ML00010 — Cold Cracks in a Gouged Weld MetalM - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
After grinding to remove the cracks, it was possible to see that they originated in the root, with longitudinal and transverse cracking, and localized in the weld metal only.
167
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Aspect by NDTDf - Cracking
Acetate metallographic replica from the surface, before cracking removal, showing the intergranular morphology of the cracks in a very refined weld metal structure.
123
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital etched, OMDf - Intergranular Cracking
Detail of the acetate metallographic replica from the surface, before cracking removal, showing the (previous austenite) intergranular morphology of the cracks in a very refined weld metal structure.
107
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital etched, OMDf - Intergranular Cracking
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

+10 more from this case →