Fabrication Defect

3 cases · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Fabrication Defect — sub-branches

Quenched and tempered structure of the F22 steel forging, presenting about 230HV10 average hardness.
133
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Left Side
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

More from these cases

ML00072 — Liquation Cracks in a High Strength JointM - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Left Side
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Right Side
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Right Side
ML00010 — Cold Cracks in a Gouged Weld MetalM - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal