Corrosion

2 cases · 11 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Corrosion — sub-branches

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
A small sample was removed from the steam drum and the micrography shows that the cracks are intergranular (previous austenite) and located in the weld metal.
285
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking

More from these cases

ML00019 — Transgranular SCC in Boiler Steam DrumM - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
Micrographic detail of the transgranular stress corrosion cracking.
157
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack
ML00020 — Intergranular SCC in Boiler Steam Drum RepairM - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
The micrography of the small sample removed from the steam drum shows that the cracks are intergranular (previous austenite) and located in the weld metal.
274
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Secondary cracks in the weld metal showing an intergranular morphology. Stress Corrosion Cracking.
249
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the secondary cracks in the weld metal with intergranular morphology. Stress Corrosion Cracking.
251
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the intergranular stress corrosion cracking of the drum shell weld repair.
217
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking