Surface Aspect

15 cases · 30 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Surface AspectDf - Corrosion
Visual aspect of the internal side of the tube, after longitudinal cut, presenting the region of leakage.  The tube, that is 1.6mm thick, presented several points of localized diissolution .
457
ML00170 / Sep.2020
MIC in Aluminum Brass Tubes
M - Aluminum BrassP - Seamless tubeAp - MaritimeCd - Preferential Dissolution
Cm - Surface AspectDf - Localized Thinning
Aspect of the external tube surface after cleaning. It is possible to see that the cracks are longitudinal to the tube and localized in positions where the surface is corroded.
132
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - Surface AspectDf - External Surface
ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Low Mag
ML00144 / Aug.2018
Impact of a .380 Winchester on Ti64 Plate
M - Ti6Al4VP - Rolled PlateAp - StructureCd - Non-Pierced
Cm - Surface AspectDf - Low Mag
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Low Mag
ML00142 / Aug.2018
Impact of a .308 Winchester on AR500 Plate
M - Low Alloy Wear ResistantP - Rolled PlateAp - StructureCd - Non-Pierced
Cm - Surface AspectDf - Low Mag
Aspect of the tubesheet after removal of the cooper alloy tubes and water cleaning. The corrosion is more intense in the regions of tube connection.
176
ML00125 / Mar.2018
Dezincification of a Cooler Tubesheet
M - BrassP - PlateAp - ShipCd - Preferential Dissolution
Cm - Surface AspectDf - Corrosion

More from these cases

ML00184 — Dissimilar Steels in a Threaded ConnectionM - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Surface AspectDf - Corrosion
ML00170 — MIC in Aluminum Brass TubesM - Aluminum BrassP - Seamless tubeAp - MaritimeCd - Preferential Dissolution
ML00170 / Sep.2020
MIC in Aluminum Brass Tubes
M - Aluminum BrassP - Seamless tubeAp - MaritimeCd - Preferential Dissolution
Cm - Surface AspectDf - Localized Corrosion
ML00170 / Sep.2020
MIC in Aluminum Brass Tubes
M - Aluminum BrassP - Seamless tubeAp - MaritimeCd - Preferential Dissolution
Cm - Surface AspectDf - Internal Surface
ML00165 — SCC of Aluminum Bronze Heating CoilM - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Aspect of the internal tube surface after a longitudinal cut, without cleaning.  It is possible to see a clean surface inside the tube.
104
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - Surface AspectDf - Internal Surface
ML00165 / Jul.2020
SCC of Aluminum Bronze Heating Coil
M - Aluminum BronzeP - Seamless tubeAp - Oil and GasCd - Stress Corrosion
Cm - Surface AspectDf - General View
ML00145 — Impact of a .380 Winchester on 6061 T6 PlateM - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Low Mag
ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Plastic Deformation
ML00144 — Impact of a .380 Winchester on Ti64 PlateM - Ti6Al4VP - Rolled PlateAp - StructureCd - Non-Pierced
ML00144 / Aug.2018
Impact of a .380 Winchester on Ti64 Plate
M - Ti6Al4VP - Rolled PlateAp - StructureCd - Non-Pierced
Cm - Surface AspectDf - Low Mag
ML00144 / Aug.2018
Impact of a .380 Winchester on Ti64 Plate
M - Ti6Al4VP - Rolled PlateAp - StructureCd - Non-Pierced
Cm - Surface AspectDf - Melted film
ML00143 — Impact of a .308 Winchester on A36 PlateM - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Low Mag
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Plastic Deformation
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Surface AspectDf - Melted film