Optical Microscope

10 cases · 99 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

A small sample was removed from the steam drum and the micrography shows that the cracks are intergranular (previous austenite) and located in the weld metal.
285
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Transverse section of the 1/16" thick tube at the autogenous seam weld.
588
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Autogenous Weld

More from these cases

ML00020 — Intergranular SCC in Boiler Steam Drum RepairM - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
The micrography of the small sample removed from the steam drum shows that the cracks are intergranular (previous austenite) and located in the weld metal.
274
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Secondary cracks in the weld metal showing an intergranular morphology. Stress Corrosion Cracking.
249
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the secondary cracks in the weld metal with intergranular morphology. Stress Corrosion Cracking.
251
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the intergranular stress corrosion cracking of the drum shell weld repair.
217
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
ML00026 — Autogenous Seam Welded Tube in Ferritic SSM - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Longitudinal Section
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Equiaxial Grains
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Ferrite
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Transverse Section
ML00026 / Feb.2017
Autogenous Seam Welded Tube in Ferritic SS
M - Ferritic Stainless SteelP - Fabrication WeldAp - AutomotiveCd - Typical manufacturing
Cm - Kalling Etched Micrography by OMDf - Equiaxial Grains

+5 more from this case →