Optical Microscope
2 cases · 14 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Optical Microscope — sub-branches

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks
More from these cases

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Transgranular Crack

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Micrography by OMDf - Branched Cracks

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Branched Cracks

ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Micrography by OMDf - Branched Cracks