Atlas

11 cases · 34 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
Image by scanning electron microscopy of the metallurgically bonded interface of the internally cladded pipe. It is a seamless pipe in a low alloy steel X70 cladded by welding overlay of Alloy 625 (by automatic GTAW process). The region is a detail of the interface inside the Ni alloy weld metal, presenting columnar grains and intragranular preciptation. The pipe was heat treated before bending (solution annealing) and after bending (quenching and tempering to meet X70 grade). The microhardness of this region is higher than the value obtained out of this region, in the overlay.
657
ML00132 / May.2018
Seamless Pipe Overlaid with Alloy 625
M - LAS / Ni AlloyP - Seamless PipeAp - Oil and GasCd - Welding
Cm - Electrolytic Etch Micrography by SEMDf - Clad Interface
The scanning electron microscopy image of the internal surface of the tube in position 2 shows a localized  corrosion region with intergranular morphology, as well a crack from the corroded region.
1237
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Surface Aspect by SEMDf - Intergranular Corrosion
Detail of the fracture surface, predominantly transgranular with secondary cracks of intergranular morphology.
831
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Micrography by SEMDf - Pitting
Image by scanning electron microscopy of the metallurgically bonded interface of the composite seamless tube (carbon steel externally claded with stainless steel), in the side of the stainless steel where a strain hardening effect plus a carbide precipitation in twins is shown.  The hardness of this region (279 HV0.3) is a lot higher than the value obtained out of this region (167 HV0.3) for the same stainless steel.
814
ML00056 / May.2018
Seamless Tube Externally Cladded with SS
M - Carbon Steel / Stainless SteelP - CladdingAp - Pulp and PaperCd - Removed From Service
Cm - Electrolytic Etch Micrography by SEMDf - Clad Interface
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Regions of the pin thread presenting pitting corrosion.
635
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00132 — Seamless Pipe Overlaid with Alloy 625M - LAS / Ni AlloyP - Seamless PipeAp - Oil and GasCd - Welding
ML00132 / May.2018
Seamless Pipe Overlaid with Alloy 625
M - LAS / Ni AlloyP - Seamless PipeAp - Oil and GasCd - Welding
Cm - Electrolytic Etch Micrography by SEMDf - Clad Interface
ML00132 / May.2018
Seamless Pipe Overlaid with Alloy 625
M - LAS / Ni AlloyP - Seamless PipeAp - Oil and GasCd - Welding
Cm - Electrolytic Etch Micrography by SEMDf - Clad Interface
ML00086 — Intergranular Corrosion of Sensitized 304SSM - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
The low magnification image of the internal surface of the tube, in position 2, shows several points of localized corrosion, with intergranular morphology.
193
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Surface Aspect by SEMDf - Intergranular Corrosion
ML00078 — Hydrogen Cracking of IN 718 Subsea ConnectorM - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00012 — Vibration Induced Fatigue in a 316/316L SSM - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Crack
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Pitting
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Pitting
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation

+2 more from this case →

ML00056 — Seamless Tube Externally Cladded with SSM - Carbon Steel / Stainless SteelP - CladdingAp - Pulp and PaperCd - Removed From Service
ML00056 / May.2018
Seamless Tube Externally Cladded with SS
M - Carbon Steel / Stainless SteelP - CladdingAp - Pulp and PaperCd - Removed From Service
Cm - Electrolytic Etch Micrography by SEMDf - Strain Hardened
ML00041 — Fatigue Fracture of Inconel 718 Spline ShaftM - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
ML00016 — SCC in Free Cutting 303SSM - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Regions of the localized corrosion spots associated to non metallic inclusions.
123
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Surface Aspect by SEMDf - Non Metallic Inclusions
ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Surface Aspect by SEMDf - Fracture