Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the internal side of the drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained uncleaned for a period a little longer than 1 month.
775
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Internal Surface
Aspect of the Nitronic 60 cylinder, OD 36.4mm, presenting pits at the external surface.
219
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - External Surface
The external surface of the 2" diameter pipe is rusted and the leakage is associated to “holes” that appear very small at the surface but that open a large hole in the middle of the thickness.
507
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
163
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - General View
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
125
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
ML00121 — Pitting Corrosion in a Subsea SystemM - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Aspect of the 17-4 PH rod, OD 10.6 mm, presenting deep pits at the external surface.
125
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - External Surface