Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the bolt fracture surface by scanning electron microscopy, (SEM) presenting striations that indicate a FATIGUE micromechanism.  The bolt is of a medium strength (class 8.8) low alloy steel, medium carbon, quenched and tempered.
1123
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Aspect of the fracture surface of the bolt, after cleaning with a  plastic brush.  Although there is a layer of oxides it is possible to see the intergranular morphology of the fracture, typical of a hydrogen embrittlement mechanism.
1154
ML00126 / Mar.2018
Hydrogen Fracture of Subsea Allen Bolts
M - Low Alloy Medium Carbon QTP - Coated ProductAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

More from these cases

ML00130 — Fatigue Fracture of Overloaded BoltsM - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Aspect of the fracture surface in low magnification, showing a flat aspect (associated to a fatigue fracture micromechanims) and a rough aspect (associated to a ductile fracture micromechanism).
167
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - General View
Aspect of the fracture surface by scanning electron microscopy, presenting fatigue striations micromechanism.  The bolt is a medium strength low alloy steel, medium carbon, quenched and tempered.
154
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Detailed fractographic aspect of the flat part of the bolt fracture, presenting fatigue striations.  The bolt is a medium strength low alloy steel, medium carbon, quenched and tempered.
141
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Fractographic detailed aspect of the rough part of the fracture surface, presenting ductile dimples.  This is the final fracture, by overload.
137
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Ductile Fracture
ML00126 — Hydrogen Fracture of Subsea Allen BoltsM - Low Alloy Medium Carbon QTP - Coated ProductAp - SubseaCd - Hydrogen Embrittlement
Detailed aspect of the fracture surface of the bolt, evidencing the intergranular morphology of the fracture (although with an oxide scale), typical of a hydrogen embrittlement mechanism.
114
ML00126 / Mar.2018
Hydrogen Fracture of Subsea Allen Bolts
M - Low Alloy Medium Carbon QTP - Coated ProductAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture