Welded Joint

1 case · 5 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Welded Joint — sub-branches

The morphology of the cracking in the weld metal is intergranular (in the previous austenite grain boundaries), and branched. The replication technique was adopted to define the nature of the cracks.
148
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks

More from these cases

ML00071 — Reheating Cracking of a CrMo Vessel WeldM - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Detail of the weld metal intergranular and branched cracking (in the previous austenite grain boundaries). The replication technique was adopted to define the nature of the cracks.
125
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks
The forged T presented a ferritic perlitic/bainitic structure at the surface, where the replica was conducted. The base material material hardness is 180 HB.
121
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Ferrite and Bainite
The thick wall tube presented a bainitic structure at the surface, where the replica was conducted. The base material material hardness is 167 HB.
109
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Bainite
The weld metal presented a ferritic/bainitic structure at the surface, where the replica was conducted. The weld metal hardness is 272 HB, too high for this material, suggesting lack of a suitable PWHT.
102
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Weld Metal