Crevice Corrosion in a Subsea System — Aspect Before Analysis
Raw Material — sub-branches

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Banded Structure
More from these cases

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Granular structure

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Grain refined structure

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Last Bead HAZ

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Last Bead HAZ

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainitic HAZ

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Left Side

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainite

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Micro by OM, picric acid+FeCl3+H2O etchDf - Segregated Regions

ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Segregated Regions