Crevice Corrosion in a Subsea System — Aspect Before Analysis

The fracture surface is flat, shows the graphite nodules and cleavage of the ferritic microstructure, indicating that the material have exceeded the capacity to acomodate the stress.
945
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets
The intake valve seat cylinder, manufactured in a high alloy white cast iron, presents a network of primary carbides, not degradated even after high temperature exposition during all lifetime.
632
ML00003 / Apr.2017
Cast iron Engine Valve Seats
M - White Cast IronP - Valve SeatAp - MaritimeCd - Microstructural Evolution
Cm - Micrography by OMDf - Network of Primary Carbides

More from these cases

ML00040 — Brittle Fracture of a Valve StemM - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Detail of the cleavage micromechanism.
195
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets
The cast iron microstructure is predominatly ferritic with graphite nodules.
169
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Graphite in Nodules
The micrography of the stem at the fracture region shows a flat fracture with transgranular clevage at the ferritic structure.
137
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Fracture
Micrography presenting a detail of the fracture surface opening to the graphite nodules.
139
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Fracture
ML00003 — Cast iron Engine Valve SeatsM - White Cast IronP - Valve SeatAp - MaritimeCd - Microstructural Evolution
The intake valve seat cylinder, manufactured in a high alloy white cast iron, presents a network of primary carbides, not degradated even after high temperature exposition during all lifetime.
206
ML00003 / Apr.2017
Cast iron Engine Valve Seats
M - White Cast IronP - Valve SeatAp - MaritimeCd - Microstructural Evolution
Cm - Micrography by OMDf - Network of Primary Carbides
The exhaust valve seat cylinder, manufactured in a high alloy white cast iron, presents a coalesced structure, degradated by high temperature exposition during the lifetime.
182
ML00003 / Apr.2017
Cast iron Engine Valve Seats
M - White Cast IronP - Valve SeatAp - MaritimeCd - Microstructural Evolution
Cm - Micrography by OMDf - Coalesced structure
The exhaust valve seat cylinder, manufactured in a high alloy white cast iron, presents a coalesced structure, degradated by high temperature exposition during the lifetime.
137
ML00003 / Apr.2017
Cast iron Engine Valve Seats
M - White Cast IronP - Valve SeatAp - MaritimeCd - Microstructural Evolution
Cm - Micrography by OMDf - Coalesced structure