Austenitic Stainless Steel

2 cases · 24 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the stub end, that is used in combination with a lap joint flange.  In this case it was prepared from a seam welded pipe, longitudinal, also with circunferential weld to the stub face (which means it was not flared).  The cracking is circunferential in the non painted region, not associated to any welded area.
435
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Aspect Before AnalysisDf - General View
Transverse section of the 2" diameter pipe at the pitting location.  The pipe was leaking.
1322
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Transverse Section AspectDf - Pitting

More from these cases

ML00168 — SCC of Austenitic SS Flange Stub EndM - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Aspect Before AnalysisDf - Cracking
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Longitudinal Section
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Longitudinal Section AspectDf - Multiple cracks

+10 more from this case →

ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
The external surface of the 2" diameter pipe is rusted and the leakage is associated to “holes” that appear very small at the surface but that open a large hole in the middle of the thickness.
507
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting
Micrography of a transverse section of the pipe, presenting the pitting corrosion. As polished.
310
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OMDf - Pitting

+2 more from this case →