Weld Metal
2 cases · 9 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Weld Metal — sub-branches

ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Weld Metal in the Center

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
More from these cases

ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Weld Metal

ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Weld Metal in the Cap

ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Weld Metal in the Root

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Weld Metal

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Weld Metal

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Weld Metal

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Weld Metal