Crevice Corrosion in a Subsea System — Aspect Before Analysis

Fusion line of the forging side, in the cap, showing the weld metal (to the top of the image) and the base metal (to the bottom of the image). The heat affected zone hardness is about 270HV10.
108
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Heat Affected Zone
ML00045 / Aug.2017
Subsea Tubular F6NM Martensitic SS
M - Martensitic Stainless SteelP - Fabrication WeldAp - OffshoreCd - Welding
Cm - Kalling Etched Micrography by OMDf - Heat Affected Zone

More from these cases

ML00178 — Cold cracks in Cr-Mo Welded ForgingM - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Heat Affected Zone
ML00045 — Subsea Tubular F6NM Martensitic SSM - Martensitic Stainless SteelP - Fabrication WeldAp - OffshoreCd - Welding
ML00045 / Aug.2017
Subsea Tubular F6NM Martensitic SS
M - Martensitic Stainless SteelP - Fabrication WeldAp - OffshoreCd - Welding
Cm - Kalling Etched Micrography by OMDf - Heat Affected Zone
ML00045 / Aug.2017
Subsea Tubular F6NM Martensitic SS
M - Martensitic Stainless SteelP - Fabrication WeldAp - OffshoreCd - Welding
Cm - Kalling Etched Micrography by OMDf - Heat Affected Zone