Microstructure

12 cases · 36 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
Low magnification micrography, by optical microscope, of the longitudinal section of a damaged bolt, in the center of the thickness. The microstructure is austenitic, free from carbides.
100
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
Micrography of the case, observed in the center of the thickness, showing an equiaxial granular austenitic microstructure, free from carbides.  The structure is typical of a 316 SS, in a solution annealed condition.
176
ML00122 / Feb.2018
Crevice Corrosion in a Subsea System
M - Austenitic Stainless SteelP - CaseAp - Oil and GasCd - Crevice
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, and evidences of the manufacturing process by hot forming.
179
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in the colder part of the equipment, position 1.  The material presented carbide precipitation at grain boundaries (not yet fully surrounding the grains) and at this point the tube presented no internal corrosion.
338
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
ML00095 / Sep.2017
MIC of a Riser Control Line
M - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Cm - Micrography by OM using A262 Method ADf - Austenite
Micrography of the plate material presenting a granular austenitic structure, free from precipitation.
122
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Eletrolytically Etched Micrography by OMDf - Austenite

More from these cases

ML00168 — SCC of Austenitic SS Flange Stub EndM - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
ML00168 / Aug.2020
SCC of Austenitic SS Flange Stub End
M - Austenitic Stainless SteelP - Stub EndAp - Chemical IndustryCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00157 — Bolts Under Chloride SCC ConditionsM - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Strain Hardened
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Strain Hardened
ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00122 — Crevice Corrosion in a Subsea SystemM - Austenitic Stainless SteelP - CaseAp - Oil and GasCd - Crevice
Micrographic detail of the fully austenitic granular structure of the case, in the center of the thickness.
158
ML00122 / Feb.2018
Crevice Corrosion in a Subsea System
M - Austenitic Stainless SteelP - CaseAp - Oil and GasCd - Crevice
Cm - Micrography by OM using A262 Method ADf - Austenite
ML00121 — Pitting Corrosion in a Subsea SystemM - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Nitronic 60 cylinder. Micrography of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, with some aligned non metallic inclusions.
157
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrographic detail of the longitudinal section in the center of the thickness, presenting a fully austenitic microstructure, equiaxial grains, typical of a solution annealed condition.
136
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite
Nitronic 60 cylinder. Micrography of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a shadow close to the external surface that is associated to a small layer of strain hardened structure (deformation twins).
133
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened
Nitronic 60 cylinder. Micrography of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a 0.15mm layer of strain hardened structure (deformation twins).
120
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened
Nitronic 60 cylinder. Micrographic detail of the longitudinal section close to the surface, presenting a fully austenitic microstructure, with a layer of strain hardened structure (deformation twins).
113
ML00121 / Feb.2018
Pitting Corrosion in a Subsea System
M - Austenitic / MartensiticP - Rod & CylinderAp - SubseaCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Strain Hardened

+3 more from this case →

ML00086 — Intergranular Corrosion of Sensitized 304SSM - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in position 2, where the temperature was higher and the carbide precipitation increased during service.
272
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intergranular Precipitation
Micrography of the 1.65 mm thickness tube, in the middle of the thickness of the longitudinal section.  This part of the tube is located in position 3, where intergranular and transgranular carbide precipitation occurred during service.
234
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intragranular Secondary Precipitation
Micrography of a longitudinal section of the tube in position 3, at the internal surface.  Although there is a strong precipitation, both intergranular and transgranular, the tube did not corrode at this point.
144
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intragranular Secondary Precipitation
Micrographic detail of the internal side of the tube in position 3, with a strong intergranular and transgranular precipitation, but no corrosion at this point.
153
ML00086 / Nov.2017
Intergranular Corrosion of Sensitized 304SS
M - Austenitic Stainless SteelP - Seamless tubeAp - Heat ExchangerCd - Intergranular Corrosion
Cm - Micrography by OM using A262 Method ADf - Intragranular Secondary Precipitation
ML00095 — MIC of a Riser Control LineM - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
ML00095 / Sep.2017
MIC of a Riser Control Line
M - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Cm - Micrography by OM using A262 Method ADf - Fusion Line
ML00095 / Sep.2017
MIC of a Riser Control Line
M - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Cm - Micrography by OM using A262 Method ADf - Fusion Line
ML00051 — Chloride SCC of 316 Heat Exchanger PlateM - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Micrographic detail of the austenitic microstructure of the heat exchanger plate, free from carbides that suggest the adoption of a material in a solution annealed condition, although the high hardness level indicates cold working.
109
ML00051 / Apr.2020
Chloride SCC of 316 Heat Exchanger Plate
M - Austenitic Stainless SteelP - Heat Exchanger PartAp - FPSOCd - Stress Corrosion
Cm - Eletrolytically Etched Micrography by OMDf - Austenite