Microstructure
4 cases · 14 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Microstructure — sub-branches

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

ML00149 / Dec.2018
Vibration Induced Fatigue in a Gas Piping
M - Low Carbon SteelP - Piping spoolAp - FPSOCd - Vibration Induced Fatigue
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite

ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - NaOH Electrolytic Etched MicroDf - Coarse Structure
More from these cases

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - NaOH Electrolytic Etched MicroDf - Banded Structure

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - NaOH Electrolytic Etched MicroDf - Coarse Structure

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

ML00150 / Dec.2018
Vibration Induced Fatigue in a SS Oil Piping
M - Duplex Stainless SteelP - PipingAp - FPSOCd - Vibration Induced Fatigue
Cm - Nital Etched Micrography by OMDf - Duplex structure

ML00149 / Dec.2018
Vibration Induced Fatigue in a Gas Piping
M - Low Carbon SteelP - Piping spoolAp - FPSOCd - Vibration Induced Fatigue
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Micrography by OM using A262 Method ADf - Austenite

ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - Electrolytic Etch Micrography by SEMDf - Delta ferrite