Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the external side of the connector, with a longitudinally crack of a brittle aspect. 
It is a 5/8" connector (15.8 mm).
134
ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Aspect Before AnalysisDf - General View
Draft of the completion riser after removal of the external case showing the hydraulic line position where the 316 tubing is welded by orbital autogenous GTAW to the Nitronic fitting (stab).  In the design of these hydraulic lines, the position of the cracking in the fitting is associated to a slightly bent condition of the fitting due to the misaligment of the tubing axis and the stab axis in the connector, visible in the draft.
1081
ML00095 / Sep.2017
MIC of a Riser Control Line
M - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Cm - Identification drawingDf - General View
Aspect of the fitting welded to a tubing, ND 5/8"  in a hydraulic line.  The through wall cracking is longitudinal in the fitting side.
1032
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - General View

More from these cases

ML00095 — MIC of a Riser Control LineM - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Aspect of the hydraulic line samples removed from service to be analyzed.  Tubing and welded joint (bottom sample) between the 316 tubing (left side of the sample) and the nitronic fitting (right side of the sample).   The cracking is located 10 mm far from the weld, autogenous orbital GTAW.
108
ML00095 / Sep.2017
MIC of a Riser Control Line
M - Austenitic Stainless SteelP - Fabrication WeldAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - General View