Fracture occurred during fabrication of a low carbon steel automotive part, welded by SAW process in one fillet, between a superior plate (8mm thick) and an inferior plate (12 mm thick). See the schematic drawing in the next figure.
290
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Aspect Before AnalysisDf - Fracture
Macrography showing the different regions of a pipe-to-plate fillet weld. See the schematic drawing in the next image
954
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - NItal Etched MacroDf - Fracture
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Fractography by SEMDf - Fracture
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Aspect Before AnalysisDf - Fracture
ML00010 / Oct.2017
Cold Cracks in a Gouged Weld Metal
M - Low Alloy Low Carbon QTP - Rolled PlateAp - OffshoreCd - Welding Defect
Cm - Fracture Surface AspectDf - Fish Eye

More from these cases

ML00069 — Liquation Cracks in SAW of Low Carbon SteelM - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Identification drawingDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - NItal Etched MacroDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - NItal Etched MacroDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00052 — Cold Cracks in API 5CT L80 Tube Welded to a Structural PartM - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Identification drawingDf - Fracture
ML00067 — Cold Cracks in C-Mn SAW Weld MetalM - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture