Damage
4 cases · 7 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Damage — sub-branches

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00173 / May.2021
Welding Cracks in an Aged HP Cast Fitting
M - Heat Resistant SteelP - Cast FtittingAp - PetrochemicalCd - Welding
Cm - Kalling Etched Micrography by OMDf - Base Metal

ML00061 / Apr.2017
Creep in a Seam Weld of a 304H SS Fitting
M - Austenitic Stainless SteelP - Fabrication WeldAp - Chemical IndustryCd - Creep
Cm - Micrography by OM using A262 Method ADf - Base Metal
More from these cases

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal

ML00061 / Apr.2017
Creep in a Seam Weld of a 304H SS Fitting
M - Austenitic Stainless SteelP - Fabrication WeldAp - Chemical IndustryCd - Creep
Cm - Micrography by OM using A262 Method ADf - Base Metal