Stress Corrosion

2 cases · 3 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Ferritic perlitic structure of the shell plate.
207
ML00018 / Apr.2017
SCC in Boiler Steam Drum
M - Low Carbon SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

More from these cases

ML00019 — Transgranular SCC in Boiler Steam DrumM - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
ML00019 / Apr.2017
Transgranular SCC in Boiler Steam Drum
M - CMn SteelP - Rolled PlateAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite