Crevice Corrosion in a Subsea System — Aspect Before Analysis
Scanning Electron Microscope — sub-branches

ML00172 / Mar.2021
Brittle Fracture of a LAS Valve Spring
M - Low Alloy Medium Carbon QTP - SpringAp - Oil and GasCd - Brittle Fracture
Cm - Surface Aspect by SEMDf - Corrosion

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Corrosion

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
More from these cases

ML00172 / Mar.2021
Brittle Fracture of a LAS Valve Spring
M - Low Alloy Medium Carbon QTP - SpringAp - Oil and GasCd - Brittle Fracture
Cm - Nital Etched Micrography by SEMDf - Martensite

ML00172 / Mar.2021
Brittle Fracture of a LAS Valve Spring
M - Low Alloy Medium Carbon QTP - SpringAp - Oil and GasCd - Brittle Fracture
Cm - Nital Etched Micrography by SEMDf - Martensite

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Corrosion

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - At the Surface

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture