Scanning Electron Microscope

4 cases · 10 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Scanning Electron Microscope — sub-branches

Fractographic detail of the longitudinal Charpy V testpiece,  broken at -46°C and presenting energy of 64J (the average energy of three tespieces was 70J).  The Charpy V testpiece was removed from the center of the bar. The micromechanism is quasicleavage and the test in this direction presented energy values superior than the minimum requirement of 45J.
944
ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece
Detail of the pin fracture surface, presenting both a flat aspect and a rough aspect in a shearing section of 2.5 mm width.
726
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Fracture
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
The fracture micromechanism is ductile for the pin that has been sheared in a condition of controlling the load carrying. Elongated Dimples.
453
ML00007 / Dec.2020
Free Machining Brass in Shear Pin
M - BrassP - Machined PartAp - LiftingCd - Shear
Cm - Fractography by SEMDf - Elongated Dimples

More from these cases

ML00123 — Non Qualified Superduplex for SubseaM - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Fractography of the broken Charpy V testpiece,  longitudinal, broken at -46°C and presenting energy of 64J (the average of three values was 70J).  In this direction the material presented an energy value higher than the minimum requirement of 45J.
109
ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece
Fractography of the Charpy V testpiece, transverse section, broken at -46°C and presenting energy of 20J (the average of three results was 33J).  The coarse structure and the alignement created a condition for low energy results in this specific direction, and the material did not present the minimum requirement of 45J.
103
ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece
ML00046 — Brittle Fracture of SS Shear PinM - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Fracture appearance in a sheared region, presenting a ductile morphology for the fracture micromechanism.
109
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Ductile Fracture
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Intergranular Cracking
ML00041 — Fatigue Fracture of Inconel 718 Spline ShaftM - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
ML00007 — Free Machining Brass in Shear PinM - BrassP - Machined PartAp - LiftingCd - Shear
ML00007 / Dec.2020
Free Machining Brass in Shear Pin
M - BrassP - Machined PartAp - LiftingCd - Shear
Cm - Fractography by SEMDf - Ductile Fracture