Surface Aspect by SEM

3 cases · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Microscopical aspect by scanning electron microscopy (SEM) of the external surface of a drilling tool in a position that presented localized deposits and corrosion under deposit. The deep corrosion in a short time is only possible associated to the biological growth and aggressive environment generated by the microorganisms metabolites - Microbiologically Induced Corrosion (MIC).
104
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Deposits
Aspect of the rusted surface after cleaning, showing adhered products at the surface, in regions where the passive layer was destroyed and pitting corrosion occurred.
184
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting regions of localized corrosion (in the beginning) and deposits
387
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00054 — Cutlery CorrosionM - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Detail of the rusted surface. EDS analysis inside the pitting shows a high Cl peak (the bright aspect inside the pitting), indicating that the salt over the surface was responsible for destroying the passive layer and the localized corrosion occurred.
172
ML00054 / Dec.2018
Cutlery Corrosion
M - Martensitic Stainless SteelP - Foodstuff ArticleAp - KitchenCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
ML00014 — Pitting Corrosion in 316SS PipeM - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Image of the external surface of the pipe presenting deposits where there is a localized corrosion at the surface.
326
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Corrosion
Image of the external surface of the pipe presenting the aspect of the localized corrosion by pitting.
297
ML00014 / Apr.2017
Pitting Corrosion in 316SS Pipe
M - Austenitic Stainless SteelP - Seamless PipeAp - FPSOCd - Pitting Corrosion
Cm - Surface Aspect by SEMDf - Pitting