Fractography by SEM
5 cases · 15 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Brittle Fracture

ML00131 / Apr.2018
Brittle Failure of a Soft Roller Bearing
M - Wear Resistant SteelP - Roller BearingAp - Mechanical IndustryCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Close to the External Surface

ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Fractography by SEMDf - Fracture

ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Fractography by SEMDf - Intergranular Cracking
More from these cases

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Intergranular Fracture

ML00148 / Sep.2018
Brittle Fracture of a 420 SS Barrel Nut
M - Martensitic Stainless SteelP - Barrel NutAp - LiftingCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Dimples

ML00131 / Apr.2018
Brittle Failure of a Soft Roller Bearing
M - Wear Resistant SteelP - Roller BearingAp - Mechanical IndustryCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Close to the Internal Surface

ML00131 / Apr.2018
Brittle Failure of a Soft Roller Bearing
M - Wear Resistant SteelP - Roller BearingAp - Mechanical IndustryCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Close to the Internal Surface

ML00131 / Apr.2018
Brittle Failure of a Soft Roller Bearing
M - Wear Resistant SteelP - Roller BearingAp - Mechanical IndustryCd - Heat Treatment Defect
Cm - Fractography by SEMDf - Close to the External Surface

ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece

ML00123 / Feb.2018
Non Qualified Superduplex for Subsea
M - Super Duplex Stainless SteelP - BarAp - Oil and GasCd - Not according to spec
Cm - Fractography by SEMDf - Broken Testpiece

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Fractography by SEMDf - Intergranular Cracking